I. Raw Material Inspection and Preparation
Hot-rolled steel coils are used as raw material for spiral welded steel pipes. Upon arrival at the plant, the first step is not to feed the coils into the machine, but to verify their identity.
- Material and Grade Verification: Confirm that the steel coil grade (Q235B, Q355B, L245, X42–X70, etc.) matches the MTC (Material Test Certificate), and verify the furnace batch number, chemical composition, and mechanical properties.
- Surface and Dimensional Inspection: Inspect the steel coil for thickness, width, sickle bend, towering, surface cracks, inclusions, and rust.
- Traceability and Record-Keeping: Each steel coil corresponds to a specific furnace batch number, which is entered into the production traceability system. This ensures that the serial number of every subsequent steel pipe can be traced back to its original steel coil.
- Pre-Machining Preparation: Confirm the storage, transfer, and uncoiling direction of the steel coils to prevent mix-ups.
II. Uncoiling and Leveling of Steel Coils
- The steel coil is loaded into the uncoiler and gradually unrolled into a steel strip.
- The strip passes through a multi-roll leveling machine to eliminate any bending memory in the coil and ensure the strip remains flat.
- The strip edges are inspected for notching, burrs, or folds; the surface is checked for indentations or uneven scale removal.
- The flatness of the strip directly affects subsequent forming operations: if the leading edge is warped or misaligned, misalignment and unstable weld gaps will occur during forming.


III. Milling and Preparation of Steel Strip Edges
Both edges of the steel strip must undergo edge milling or planing:
- To control edge straightness and width accuracy;
- To produce a groove shape that meets welding requirements (typically approximately square or slightly V-shaped);
- To remove burrs, oil, and scale from the edges;
- To ensure a uniform weld gap during butt welding.
The quality of the groove and edges directly determines the penetration depth and weld bead formation. If the edges are not clean, porosity, slag inclusion, and lack of fusion are likely to occur during welding.
IV. Spiral Forming
This is the key process that distinguishes spiral-welded steel pipes from straight-seam welded steel pipes.
1. Forming Principle
Steel strips are fed into the forming line at a specific helix angle and are continuously bent by multiple sets of rollers to form a spiral pipe blank. Steel strips of the same width can produce steel pipes with different outer diameters by adjusting the helix angle.
- The helix angle is typically adjusted within the range of 30° to 70°;
- the pipe diameter is primarily determined by the steel strip width and the helix angle;
- during the forming process, the edge misalignment, weld gap, and tube roundness are controlled in real time.
2. Key Control Points
- Weld Gap: Generally maintained between 1 and 3 mm; if too large, the weld will not penetrate fully; if too small, it may cause the torch to bump or result in undercut.
- Misalignment: Typically required to be ≤1.5 mm; exceeding this tolerance will cause a shift in the stress distribution within the weld.
- Roundness and Outer Diameter: These are adjusted in-line via forming and finishing rolls to ensure compliance with standard tolerances.
- Tension Control: A stable tension must be maintained during steel strip conveyance to prevent fluctuations in forming.
3. Impact on Quality
Molding instability directly leads to:
- Misalignment of weld seams;
- Excessive ovality in steel pipes;
- Frequent adjustments to welding parameters;
- Difficulties in subsequent pipe cutting, beveling, and on-site butt welding.
V. Internal and External Submerged Arc Welding
1. What Is Double-Sided Submerged Arc Welding (DSAW)?
Submerged arc welding (SAW) refers to a process in which an electric current is applied to the welding wire beneath a layer of flux to initiate the arc. The arc is covered by the flux and does not come into contact with the air; therefore, the weld produces a clean weld bead, minimal spatter, and deep penetration.
Spiral welded pipes are manufactured using double-sided submerged arc welding:
- Internal welding: A weld is first applied inside the pipe to form the weld from the inside;
- External welding: A weld is then applied to the outside of the pipe to achieve the required penetration from the outside;
- The internal and external welds overlap in the thickness direction, resulting in full-cross-sectional fusion.
2. Welding Sequence
The typical sequence is to weld the inner side first, followed by the outer side. Welding the inner side ensures proper back-side contour, while welding the outer side ensures adequate penetration and the desired external bead height. For thick-walled sections, multi-wire and multi-pass welding may be used.
3. Key Welding Parameters
| Parameter | Typical Range | Control Purpose |
|---|---|---|
| Welding Current | 600–1000 A | Determines penetration depth |
| Arc Voltage | 28–34 V | Affects weld width and bead formation |
| Welding Speed | 0.8–1.5 m/min | Affects heat input |
| Wire/Flux Matching | Matched to the steel grade | Ensures strength and toughness |
Mismatched parameters can result in:
- Insufficient current → Incomplete fusion, lack of penetration;
- Excessive current → Burn-through, undercut, embrittlement of the heat-affected zone;
- Excessive speed → Poor weld bead formation;
- Moisture in the flux → Porosity, hydrogen-induced cracks.
4. Why Must Both Sides Be Welded?
If only one side is welded, the root of the weld is prone to lack of fusion and slag inclusion; double-sided welding ensures fusion throughout the entire thickness of the weld, resulting in more reliable pressure-bearing capacity and fatigue performance. This is also the fundamental prerequisite for the use of SSAW in medium- and high-pressure transmission pipelines.
VI. Steel Pipe Cutting and End Machining
Welded spiral pipes are continuous, long sections that must be cut to specific lengths:
- Common standard lengths are 6 m and 12 m, though custom lengths can be provided as specified in the contract;
- Cutting is typically performed using plasma or oxy-fuel cutting;
- After cutting, inspect the cut surface to ensure it is smooth and free of slag;
- Pipe ends are machined to standard bevels (typically 30°–35°) to ensure the quality of on-site butt welding;
- Re-measure the length and end face perpendicularity to prevent misalignment during installation.
Poor bevel quality can easily lead to lack of root penetration during on-site welding, making this a high-risk area for potential engineering hazards.
VII. Non-Destructive Testing and Quality Inspection
1. Ultrasonic Testing (UT)
- Purpose: To screen for internal defects in welds, such as lack of fusion, lack of penetration, slag inclusions, and cracks.
- Timing: Continuous in-line inspection immediately after welding, covering the entire spiral weld.
- Features: Fast, radiation-free, and suitable for 100% in-line screening.
- Evaluation: An automatic alarm sounds and a mark is sprayed upon detection of an anomaly; a subsequent manual re-evaluation is conducted.
2. Radiographic Testing (RT)
- Purpose: To visually confirm areas identified as suspicious by UT, T-joints, and pipe end welds.
- Timing: Offline or online re-inspection; not all pipes undergo 100% radiographic testing.
- Characteristics: Intuitive, but costly and inefficient.
- Evaluation: Grades are assigned according to product standards; Grade II is typically considered acceptable, and cracks or lack of fusion are not permitted.
3. Visual Inspection (VT)
- Inspect for weld bead height, undercut, spatter, surface cracks, spatter marks, misalignment, etc. The weld bead height is generally controlled between 0 and 3 mm, with a smooth transition to the base metal.
4. Hydrostatic Pressure Test
- Purpose: To verify the overall pressure integrity and tightness of the steel pipe.
- Pressure Calculation: Calculated using the standard formula P = 2 × S × t / D or as specified in the contract; typically higher than the design pressure.
- Pressure Holding Time: Determined based on standards and pipe diameter; generally no less than 5–10 seconds, with longer durations required for high-pressure pipes.
- Pass/Fail Criteria: The test is considered passed if there are no leaks, no permanent deformation, and the pressure remains stable.
- Recording: The pressure-time curve is automatically saved and traceable.
- Key Point: Ultrasonic testing (UT) detects “defect signals,” while the hydrostatic test verifies “whether the pipe can withstand pressure.” The two cannot be used as substitutes for one another.
5. Defect Correction and Reinspection
- Automatically mark the defect location;
- After manual verification, grind or repair the weld;
- The repaired area must undergo UT/RT and hydrostatic testing again;
- The number of repairs allowed for a single weld is limited by the standard; any excess results in rejection.
6. The inspection ratio depends on the standard
- GB/T 9711 (Oil and Gas Pipes): Typically 100% UT; RT is performed on a proportional basis or as a full inspection;
- SY/T 5037 (General-Purpose Fluid Pipes): Full UT inspection; RT may be performed on a sampling basis;
- API 5L: NDT and hydrostatic testing requirements are specified based on the PSL grade and the contract.
The procurement documents must clearly specify: “which standard applies, which PSL level, the UT/RT ratio, and the hydrostatic test pressure”; otherwise, the manufacturer will perform testing using the minimum required configuration.
VIII. Dimensional Inspection and Final Quality Control
After testing is complete, perform a final dimensional and visual inspection on each pipe individually:
- Outer diameter: Measured using the circumference method or calipers;
- Wall thickness: Measured using ultrasonic thickness gauges or micrometers, with particular attention to minimum wall thickness;
- Length: Deviation from specified length;
- Ovality: Roundness of the pipe end cross-section;
- Straightness: Bending along the entire length;
- End face perpendicularity and bevel: Affects on-site assembly;
- Numbering and Markings: Verify pipe number, furnace batch number, steel grade, and standard.
Pipes are only transferred to the finished goods area if all dimensions, appearance, testing results, and documentation meet the requirements.
IX. Marking, Packaging, and Shipping
- Pipe Body Marking: Specifications, steel grade, standard, furnace batch number, pipe number, and production date;
- Pipe End Protection: Plastic caps or steel end caps to prevent foreign objects from entering;
- Stacking: Stack in layers with spacers to prevent coating damage and pipe deformation;
- Lifting: Use nylon slings or specialized lifting equipment; do not use steel wire ropes to directly constrict the pipes;
- Loading and Securing: Prevent rolling during transport and damage to the coating;
- Accompanying Documentation: MTC, NDT reports, hydrostatic test records, dimensional reports, and certificates of conformity.
Shipment is not the end of the process; the completeness of the documentation determines whether on-site acceptance can proceed smoothly.
X. Frequently Asked Questions (FAQ) for Procurement and Engineering Personnel
1. How are spiral welded steel pipes manufactured?
Steel coil → Uncoiling and leveling → Edge milling → Spiral forming → Internal and external submerged arc welding → In-line non-destructive testing → Cutting to length → Hydrostatic testing → Final dimensional inspection → (Corrosion protection) → Marking and shipment.
2. What welding method is used for 24 Inch SSAW Steel Pipe?
Submerged arc welding (SAW) is used, typically double-sided submerged arc welding: the inner side is welded first, followed by the outer side. The flux covers the arc, ensuring stable weld quality and deep penetration.
3. Why is it necessary to weld both the inner and outer sides?
Single-sided welding is prone to lack of fusion and slag inclusion at the root. Double-sided welding ensures full-thickness fusion along the entire weld, providing more reliable pressure resistance and meeting the requirements for medium- and high-pressure pipelines.
4. How is the outer diameter of spiral-welded pipes controlled?
This is primarily achieved by adjusting the steel strip width, the helix angle, and the forming rolls. In-line diameter measurement and edge misalignment control ensure that the outer diameter and roundness remain within tolerance limits.
5. Do all spiral-welded pipes require hydrostatic testing?
This depends on the product standards and the contract. High-pressure oil and gas pipes are typically hydrostatically tested on a per-pipe basis; ordinary low-pressure water pipes also often require per-pipe testing; however, the specific proportion and method must be specified in the procurement technical specifications.
6. At what stage is the anti-corrosion coating applied?
After the steel pipe body has passed inspection and before shipment. First, non-destructive testing and hydrostatic testing of the base pipe are completed, followed by shot blasting, heating, coating, and leak testing, and finally, end protection and packaging.